Earthenware Glazes

Please note that Lead Bisilicate and frits containing Lead Bisilicate are toxic, as are some of the other materilas used in these glazes. Care should be used in hancdling these ingredients and these glazes should not be used for functional ware. Please read the Disclaimer and Terms of Use before preceding to work with these reci[pes!

Maiolica Glaze
Cone 07-06
Oxidation
 
Ferro Frit 4364 (Lead Bisilicate - Toxic!) 
Ferro Frit 3271 (Borax Frit) 
Kaolin 
Tin Oxide
31.5 
68.5 
10 
10
 

Bleu de Sorel (Sorel blue)
Cone 04
 
E.P.kaolin 
Frit #3134 
Bentonite 

Zircopax 
Cobalt carbonate

20% 
78% 
2% 

18% 
4%

View an example of this glaze!
Thank you to Edouard Bastarache
for supplying glaze recipe and image.
 

Bleu de Ginette (Ginette's blue)
Cone 04
 
Hardwood ash (washed) 
Custer spar 
Frit #3134
E.P.kaolin
Lithium carbonate 

Bentonite
Ultrox
Cobalt oxide

35% 
14%
25% 
14% 
12%

2% 
15% 
5%

View an example of this glaze!
Thank you to Edouard Bastarache
for supplying glaze recipe and image.
 

Edouard's Vert jade cendré (Jade green ash glaze)
Cone 04
 
Hardwood ash (washed)
Custer spar
Frit #3134
E.P.kaolin
Lithium carbonate

Bentonite
Ultrox
Black copper oxide

36%
14.5%
23%
14.5%
12% 

2%
15.5%
3.5% 

View an example of this glaze!
Thank you to Edouard Bastarache
for supplying glaze recipe and image.
 

Maiolica Glaze
Cone 04
Oxidation
 
Ferro Frit 4364 (Lead Bisilicate - Toxic!) 
Kaolin 
Whiting 
Silica 
Tin Oxide
74 
10 
2 
4 
10
 

Clear Gloss
Cone 08 - 04
Oxidation
 
Ferro Frit 4110 
Whiting 
Kaolin
85.0 
5.0 
10.0
 

Clear Gloss
Cone 04
Oxidation
 
Ferro Frit 3124 
Ball Clay
85.0 
15.0
Comments: Goes well to 1120 C. Apply thinly or may go milky.
 
 

Clear Gloss
Cone 04
Oxidation
 
Frit 4064 (Lead Bisilicate - Toxic!)  
Kaolin 
Silica 
Whiting
78.0 
13.5 
4.5 
4.0
Not suitable for tableware!
 
 

Matt Clear E/W
Cone 04
Oxidation
 
Potash Feldspar 
Silica 
Colemanite 
Whiting 
Barium Carbonate (Toxic!) 
Zinc Oxide
46.8 
10.0 
11.0 
13.0 
13.0 
4.0
Not suitable for tableware!
 
 

Semi Opaque Tan/Cream E/W
Cone 04 - 03
Oxidation
 
Calcium Borate Frit  (Lead Bisilicate - Toxic!) 
Rutile 
Bentonite 
Silica 
Potash Feldspar
8.0 
60.0 
8.0 
4.0 
4.0 
16.0
Not suitable for tableware!
 
 

Aqua Blue Dry Glaze
Cone 2 - 4
Oxidation
 
Nephelene Syenite 
Barium Carbonate (Toxic!) 
Ball Clay 
Zinc Oxide 
Black Copper Oxide
40.0 
30.0 
15.0 
5.0 
4.0
Comment: Fast cooling helps preserve color.
 
 

Transparent Flowing Glaze
Cone 04
Oxidation
 
Lead Bisilicate (Toxic!) 
Kaolin 
Nephelene Syenite
76.5 
8.0 
15.5
Comment: variations can be achieved by adding small amounts of oxides and carbonates ( 2-5%).
Not suitable for tableware!
 

Bright Bronze
Cone 03
Oxidation
 
Ferro Frit 4508 
Ferro Frit 4363 
Kaolin 
Potash Feldspar 
Manganese Dioxide 
Copper Oxide 
Nickel Oxide 
Titanium Oxide
8.8 
69.0 
3.0 
9.0 
7.6 
1.0 
1.4 
0.2
Not suitable for tableware!
 


Disclaimer: It is the responsibility of anybody using the supplied glaze recipes to be informed of glaze dangers and to ensure the proper safety precautions are met when mixing and using glazes. In general glaze components marked 'toxic!' should not be used for tableware. Othert unmarked ingredients may be harmful to health on skin contact or if ingested. Frits may contain Lead Bisilicate. General safety precautions for ceramic materials apply. Contact a supplier, lecturer or professional if in doubt. Neither Ceramics Today nor its Guide Steven Goldate will bear any responsibility for incorrectly used glazes and/or ingredients, nor for any damages due to unexpected glaze results. All glazes should be tested before use.

 