Earthenware Glazes
(Printer Friendly
Version)
brought to you by
Ceramics Today
Please note that Lead Bisilicate and frits containing Lead Bisilicate are toxic, as are some of the other materilas used in these glazes. Care should be used in handling these ingredients and these glazes should not be used for functional ware. Please read the Disclaimer and Terms of Use before preceding to work with these reci[pes!
Maiolica Glaze
Cone 07-06
Oxidation
| Ferro Frit 4364 (Lead Bisilicate - Toxic!) Ferro Frit 3271 (Borax Frit) Kaolin Tin Oxide |
31.5 68.5 10 10 |
Bleu de Sorel (Sorel blue)
Cone 04
| E.P.kaolin Frit #3134 Bentonite Zircopax |
20% 78% 2% 18% |
Bleu de Ginette (Ginette's blue)
Cone 04
| Hardwood ash (washed) Custer spar Frit #3134 E.P.kaolin Lithium carbonate Bentonite |
35% 14% 25% 14% 12% 2% |
Edouard's Vert jade cendré (Jade green ash glaze)
Cone 04
| Hardwood ash (washed) Custer spar Frit #3134 E.P.kaolin Lithium carbonate Bentonite
|
36% 14.5% 23% 14.5% 12% 2% |
Maiolica Glaze
Cone 04
Oxidation
| Ferro Frit 4364 (Lead Bisilicate - Toxic!) Kaolin Whiting Silica Tin Oxide |
74 10 2 4 10 |
Clear Gloss
Cone 08 - 04
Oxidation
| Ferro Frit 4110 Whiting Kaolin |
85.0 5.0 10.0 |
Clear Gloss
Cone 04
Oxidation
| Ferro Frit 3124 Ball Clay |
85.0 15.0 |
Clear Gloss
Cone 04
Oxidation
| Frit 4064 (Lead Bisilicate
- Toxic!) Kaolin Silica Whiting |
78.0 13.5 4.5 4.0 |
Matt Clear E/W
Cone 04
Oxidation
| Potash Feldspar Silica Colemanite Whiting Barium Carbonate (Toxic!) Zinc Oxide |
46.8 10.0 11.0 13.0 13.0 4.0 |
Semi Opaque Tan/Cream E/W
Cone 04 - 03
Oxidation
| Calcium Borate Frit
(Lead Bisilicate - Toxic!) Rutile Bentonite Silica Potash Feldspar |
8.0 60.0 8.0 4.0 4.0 16.0 |
Aqua Blue Dry Glaze
Cone 2 - 4
Oxidation
| Nephelene Syenite Barium Carbonate (Toxic!) Ball Clay Zinc Oxide Black Copper Oxide |
40.0 30.0 15.0 5.0 4.0 |
Transparent Flowing Glaze
Cone 04
Oxidation
| Lead Bisilicate (Toxic!) Kaolin Nephelene Syenite |
76.5 8.0 15.5 |
Bright Bronze
Cone 03
Oxidation
| Ferro Frit 4508 Ferro Frit 4363 Kaolin Potash Feldspar Manganese Dioxide Copper Oxide Nickel Oxide Titanium Oxide |
8.8 69.0 3.0 9.0 7.6 1.0 1.4 0.2 |