Mid Fire Glazes
(Printer Friendly Version)
brought to you by
Ceramics Today
Edouard's Bleu marbré cendré
(Mottled blue ash glaze)
Cone 4
| Nepheline/Syenite Hardwood ash(washed) Silica Ball clay Gerstley borate Bentonite |
25% 20% 20% 5% 30% 2% |
Edouard's Brun veiné cendré
(Mottled brown ash glaze)
Cone 4
| Nepheline/Syenite Silica Hardwood ash (washed) Lithium carbonate Ferro Frit #3134 Bentonite Sorelslag |
35% 16% 27% 3% 10% 3% 12% |
Steve's Brilliant Ink Blue
Cone 4
Oxidation or Reduction
| Ferro Frit 3134
Potash Feldspar Ball Clay Zinc Oxide (dense) Cobalt Carbonate Cobalt Oxide |
50.0 20.0 20.0 10.0 1.5 1.5 |
Translucent Clear Gloss
Cone 4 - 5
Oxidation
| Ferro Frit 4508 Nephelene Syenite Ball Clay Tin Oxide |
60.0 20.0 20.0 6.0 |
Clear to Milky Crackle
Cone 4 - 6
Oxidation
| Lithium Carbonate Gerstly Borate Zinc Oxide (calcined) Calcium Flouride Silica Bentonite |
25.0 25.0 5.0 5.0 25.0 2.0 |
Clear Satin Matt
Cone 4 - 7
Oxidation
| Ferro Frit 4508 Potash Feldspar Ball Clay Magnesium Carbonate |
50.0 20.0 20.0 10.0 |
Smooth White Matt
Cone 4 - 7
Oxidation
| Ferro Frit 4616 Nephelene Syenite Ball Clay |
60.0 20.0 20.0 |
Clear Bright Gloss
Cone 5
Oxidation
| Gerstly Borate Silica Kaolin Potash Feldspar Bentonite |
51.0 31.0 16.0 3.0 1.0 |
Helens Matt Textured Rust
Cone 5
Neutral Gas Atmosphere
| Potash Feldspar Nephelene Syenite Dolomite Kaolin Silica Barium Carbonate Copper Carbonate |
15 20 25 5 15 5 2 |
Helens Satin Mottled Eucalyptus
Cone 5
Neutral Gas Atmosphere
| Nephelene Syenite Whiting Ball Clay Lithium Carbonate Silica Copper Carbonate |
40 25 25 5 5 2 |
| Nephelene Syenite Ferro Frit 4508 Kaolin Silica |
40.0 45.0 10.0 10.0 |
Clear Gloss
Cone 6
Oxidation
| Gerstly Borate Silica Kaolin Whiting Bentonite |
49.5 32.0 16.0 1.5 1.0 |
Clear Gloss
Cone 6
Oxidation
| Nephelene Syenite Magnesium Carbonate Zinc Oxide Kaolin Silica Bentonite |
35.5 14.6 11.9 2.4 35.6 1.0 |
Clear Gloss
Cone 6
Oxidation
| Nephelene Syenite
Gerstly Borate Silica Kaolin Bentonite |
46.2 28.0 20.4 5.4 1.0 |
Clear Gloss
Cone 6
Oxidation
| Volcanic Ash Ferro Frit 3134 Koalin Bentonite |
63.7 27.3 9.0 1.0 |
Helens Satin Brilliant Blue
Cone 6-7
Neutral Gas Atmosphere
| Potash Feldspar Nephelene Syenite Zinx Oxide Silica Barium Carbonate Cobalt Oxide |
15 20 20 5 40 0.7 |
Translucent Clear
Cone 6 - 7
Oxidation
| Potash Felspar Calcite Silica Ball Clay Ferro Frit 4508 Barium Carbonate |
25.0 20.0 35.0 25.0 20.0 10.0 |
| Volcanic Ash Ferro Frit 3134 Kaolin Kaolin (calcined) Bentonite |
52.5 28.0 5.3 4.0 2.0 |
| Ababi's Cone 6 Glazes FALLS CREEK SHINO ABABI.#6 Cone 6 FRIT 3134 40.00 Seger Weight% You can try it with any red clay. This recipe substitutes a recipe
with lithium carbonate. SUPERCRAWL AVERAGE 4 Cone 6 Cryolite 15.00 Seger Weight% And SUPERCRAWL #6 Cone 6 1201 deg.C. - Nepheline Syenite 10.00 Seger Weight% Both recipes must be like "sour cream". You better add CMC just before use, apply several times until the glaze crakles (i.e. before the firing). The CMC will help it to stay on the ware. As times passes you will learn how much or which of the two you prefare. I like #6 PLASTIC TOUCH Cone 6 1201 deg.C. - STRONTIUM CARBONATE 23.00 Seger Weight% ABABI'S CONCRET FOR ^6 Cone 6 1201 deg.C. - Portland Cement 22.00 Seger Weight% A kind of silky clear mottled glaze ( the fluor in the cryolite has a mottling efect) While firing the fluor fumes are not healthy! Make as much as you need for one session. Looks different thin or thick! |